Bubbles in Middle of Safety Laminated Glass of CNC-Shield(R) Polyvinyl Butyral PVB

Bubbles in Middle of Safety Laminated Glass of CNC-Shield® Polyvinyl Butyral PVB

CNC-Shield® Polyvinyl Butyral PVB
Reason Possibility 1:
In the procedure of roller exhausting air, it’s too early to seal the
edges of the pre-laminated glass, so the air can not be exhausted out
completely in the second roller.

Solution:
Adjust the speed and temperature in the pre-laminating procedure, make
sure the pre-laminated glass is not sealed before the second roller
exhausting air stage. Or adjust the speed of and temperature of the
silicone rubber ring, to make sure the air is totally exhausted out.
Reason Possibility 2:
The Polyvinyl Butyral PVB interlayer film already absorbed too much moisture.

Solution:
Check the moisture of the Polyvinyl Butyral PVB interlayer film, and
the humidity of the laminating room and glass surface.

Reason Possibility3:
The plainness of the tempered glass is not good enough.
Solution:
Choose good quality tempered glass, or use thicker Polyvinyl Butyral
PVB interlayer film.